Skip to main content

Table 6 Geopolymer Physical Properties (L/S 0.26, KOH 10 M, curing at ambient temperature, curing time 28 d)

From: Sustainable solidification of ferrochrome slag through geopolymerisation: a look at the effect of curing time, type of activator and liquid solid ratio

Geopolymer

GP0

GPS1

GPA2

Mass of geopolymer (g)

350.46

360.64

362.27

Mass of cast after 24 h soak (kg)

399.45

390.35

385.13

Open porosity

0.39

0.24

0.18

UCS (MPa)

12.9

14.7

24.5

UCS (MPa) after 24 h soak

3.9

8.7

19.9

Water absorption %

14.0

8.2

6.3